Non Alloy Structural Steel to EN 10025:2004 S275 Standard
Use:
The S275steel specification covers several grades of carbon steel plates for
general application such as coldforming, i.e. bending, folding,
bordering and flanging.
The steel grades of the JR, JO and J2 categories are in general suitable for all welding techniques.
S275 Chemical Properties under EN 10025:2004 (Cast Analysis)
S275JR
S275J0
S275J2
Carbon,
max
0.21
0.18
0.18
Manganese,
max
1.50
1.50
1.50
Phosphorus,
max
0.035
0.030
0.025
Sulphur,
max
0.035
0.030
0.025
Cu,
Max
0.55
0.55
0.55
S275 Mechanical Properties
S275JR/JO/J2
Tensile
Strength:
[410-580 MPa]
59,000- 84,000 psi
Min.
Yield Point:
[275 MPa] 40,000psi
We can supply:
Thickness from 6mm to 150mm (although thicker plates might be manufactured under special order)
Width: from 1,500mm to 4,100mm
Length: from 6,000mm to 20,000mm
Symbols used in EN 10025-2:2004 non-alloy structural steels
Example: S235JR+AR, S235J2C+N
S: Structural steel.
E: Engineering steel.
235: Minimum yield strength (Reh) in MPa at 16mm
JR: Longitudinal Charpy V-notch impacts 27 J at + 20°C
J0: Longitudinal Charpy V-notch impacts 27 J at 0°C
J2: Longitudinal Charpy V-notch impacts 27 J at - 20°C
+AR: Supply in as rolled conditions
+N: Supply in normalized/normalised rolled conditions
Customer options
C: Grade suitable for cold forming
Z: Grade with improved properties perpendicular to the surface